High quality Hastelloy C-276 600# Vacuum castings UNS N10276 W.Nr.2.4819 NiMo16Cr15W

Description

chemical composition

C

Si

S

P

Mn

V

≤0.01

≤0.08

≤0.001

≤0.015

≤1.0

0.1-0.3

Cr

Ni

Co

Mo

Fe

W

15.0-16.5

Bal

≤2.50

15.0-17.0

4.0-7.0

3.0-4.5

 

Mechanical properties (Standard)

shape

θ/℃

σЬ/ MPa

σ0.2/MPa

δ5 /%

Pipe

20

≥727

≥313

≥70

Plate

20

≥741

≥347

≥67

Bar

20

≥758

≥363

≥62

Belt

20

≥796

≥376

≥60

Physical property:
Solute point:1325-1370 ℃

Density:8.90 g/cm3

 

Physical quantity: 

Θ/℃

thermal conductivity W/mk

electric resistance

μΩcm

springform KN/mm2

20

10.6

125

208

100

12

127

204

300

15.4

129

195

500

17.1

129

182

600

20.7

128.5

175

700

22.6

128

168

800

24.3

126.5

160

900

26.2

126

151

1000

28

125.5

143